2.CBN grinding wheel in the hole in the application Internal
grinding efficiency
has been very low, the main reason is the grinding
speed, grinding wheel
material and the rigidity of the problem.Production
process used in dressing
wheel, grinding wheel replacement time
accounted for almost a single piece of
work time1/3 to 1/5.If
the inner or groove grinding using CBN electroplated
grinding wheel,
and the wheel speed, increasing the diameter of the grinding
rod,can be
properly increased workpiece speed and feed rate, not only can
guarantee the hole (arc) diameter, groove width size and shape
Bit accuracy,
surface roughness and avoid burns, but also can be
doubled to improve processing
efficiency and reduce processing costs.Such
as a domestic factory processing
an annual output of 600,000 textile
machinery rolling bearing sets, grinding
φ15.5 +0.04 the hole and the
adjacent arc groove, in the past with chrome
corundum (GG) wheel, need
to use two processes in two M224
internal grinding
machine, the slot (arc) diameter difference and the
size and hole concentricity
is difficult to ensure, and low efficiency,
the use of CBN wheel, the coarse
grinding rod, increased feed, saving
trim And
then changed to hole, groove at the
same time grinding, that is, in the
grinding rod installed two grinding wheel,
so that the grinding
efficiency increased by 1 times, saving a grinding
machine.The
surface roughness of the workpiece is Ra0.63μm. The grinding process
parameters are as follows: υ = 36m / s, υ2 = 19m / min, f = 1μm / r, f =
0.5μm / r,Time t = bs, with 10% concentration of the emulsion value.